1.2311 Tool steel

Our selected range provides the right material for any application.

Products

Characteristics

Designation

Strength

280–325 HB
(≈ 950–1,100 N/mm²)

Chemical composition

Thermal conductivity at 100 °C

35 W/(mK)

Character

Alloyed, quenched and tempered tool steel, especially suitable for polishing
High dimensional stability

Application

Machining

Suited:
Etching, EDM

Polishing:
Good polishability; for higher surface requirements we recommend steels for through hardening

Nitriding:
Increases the steel’s wear resistance

Hard chrome plating:
Increases the steel’s wear resistance and particularly its corrosion resistance

Use

Cavity plates, mould inserts and high-strength machine parts

Heat treatment

Already pre-hardened; usually no heat treatment required

Nitriding:
Before nitriding, stress-relieving heat treatment is recommended at 580 °C (Meusburger standard).

Hard chrome plating:
After the hard chrome plating, the mould must be tempered about 3 to 4 hours at 180 °C to avoid brittle fractures from hydrogen.

Hardening:
840 to 860 °C

Cooling:
To about 180/220 °C in oil / hot bath, then in air to about 100 °C
Obtainable hardness: 52 HRC

Tempering:
Slow heating to tempering temperature immediately after hardening
Minimum time in furnace: 1 hour per 25 mm part thickness

Technical tip

Core strength decreases with increasing plate thickness ⇒ for thickness > 300, 1.2738 is recommended

Choix boutique

Construction d’outils de découpe
Construction d’outils de découpe
Construction de machines et de gabarits
Construction de machines et de gabarits

Aperçu du panier

Aperçu CAD

Votre panier est vide.
Montant net
Vers le panier