1.2738 Tool steel

Our selected range provides the right material for any application.

Products

Characteristics

Designation

Strength

280–325 HB
(≈ 950–1,100 N/mm²)

Chemical composition

Thermal conductivity at 100 °C

33.5 W/(mK)

Character

Low-sulphur tool steel, supplied in quenched and tempered condition
Uniform hardness even with maximum dimensions, thanks to the nickel content

Application

Machining

Ideally suited:
Polishing, EDM, nitriding, etching

Suited:
Hard chrome plating

Use

Large cavity plates with deep cavities for items such as bumpers or dashboards, moulding frames

Heat treatment

Already pre-hardened; usually no heat treatment required

Soft annealing:
710 to 740 °C, about 2 to 5 hours
Slow controlled cooling inside the furnace of 10 to 20 °C to about 600 °C
Further cooling in air, max. 235 HB

Hardening:
840 to 870 °C
Maintain curing temperature for 15 to 30 minutes
Cooling in oil/hot bath/air to 180 to 220 °C
Obtainable hardness: 53 HRC

Tempering:
Slow heating to tempering temperature immediately after hardening
Minimum time in furnace: 1 hour per 20 mm part thickness
Tempering twice is recommended

Selección de la tienda

Vista previa del carrito

Vista previa CAD

Su carrito de la compra está vacío.
Total neto
Ir al carrito

Importante:

El artículo que desea configurar forma parte de un . Después de configurarlo, asegúrese de comprobar que todas las placas y componentes son compatibles desde el punto de vista técnico.