Contact

We are gladly available for you from Monday to Friday from 8:00 to 17:00. Use this link to find the contact persons for your region.

Headquarters Wolfurt
+43 5574 6706-0

Your contacts

Shopping cart {{ (warenkorbCtrl.warenkorb.bestellNummer ? (' [' + warenkorbCtrl.warenkorb.bestellNummer + '] ') : '' )}} | {{warenkorbCtrl.warenkorb.items.length}} Items   Change shopping cart

Remark

Picture Items Pcs Single price Total price Total price incl. discount
{{warenkorbItem.produktgruppe.produktname}}

{{warenkorbItem.bezeichnung | artikelBezFilter:warenkorbItem.attributwertEingaben:[{attrPrefix: 'L_', searchPattern: '/...', replacePrefix: '/', replaceSuffix: ''}] }} {{warenkorbItem.bezeichnung | artikelBezFilter:warenkorbItem.attributwertEingaben}}

{{attributwertEingabe.attributBezeichnung}}

     
{{hannexItem.Benennung}}

{{hannexItem.Bezeichnung}}

     

Please log in to see the precalculated prices and continue with the ordering process.

Lowering tension

In our selected range you can find the right material for virtually any application.

1.2738 TSHH steel for plastic moulds

DESIGNATION:

DIN:Special alloy
AFNOR:
UNI:
AISI:

INDICATORY ANALYSIS:

C0.26
Mn1.45
Cr1.25
Mo0.50
Ni1.05
V0.12

STRENGH:

33 - 38 HRC
(≈ 1050 - 1200 N/mm²)

THERMAL CONDUCTIVITY AT 250°C:

41.3W/m K


CHARACTER:

Modified, pre-toughened steel for plastic moulds, which is characterised by good polishability and optimal grainability; high thermal conductivity and wear resistance

APPLICATION:

Cavity plates without dimension restrictions, with deep cavities and high core loads


TREATMENT BY:

Polishing, etching, EDM, nitriding:
highly suitable

Hard chrome plating:
is possible


HEAT TREATMENT:


Already pre-toughened; usually no heat treatment required


Soft annealing:
720°C 1 hour per 25 mm part thickness
slow controlled cooling inside the furnace
max. 245 HB

Hardening:
880 °C
keep curing temperature for 15 to 30 minutes
cooling in hot bath/oil/compressed gas
obtainable hardness: 50 HRC

Tempering:
slow heating to tempering temperature immediately after hardening;
minimum time in furnace: 1 hour per 25 mm part thickness

TEMPERING CHART:


TECHNICAL TIP:
  • uniform hardness over the entire cross section
  • improved weldability
  • higher toughness than 1.2738

To the mould making overview To the die making overview

Available in the web shop as:
Data sheet 1.2738 TSHH

Open PDF

Material grades brochure

Material grades brochure

Material grades poster

Material grades poster

Log in

Are you already a customer?

If you already have access data for the Meusburger portal, please log in here:

Forgot your password?

The newly generated password is already on the way and should arrive soon in your inbox. We wish you a successful day.

Please enter your email address.
We will send you a new password.

Shop selection

Select your country

Locations

Try our new version of 'My account'

Get familiar with our new ‘My account’ section and benefit from numerous advantages.

Now the new ‘My account’ also gives you a direct insight into the next level of the Meusburger portal. Check out all the information and benefits of the portal here.

Get familiar with our new ‘My account’ section and benefit from numerous advantages.

Now the new ‘My account’ also gives you a direct insight into the next level of the Meusburger portal. Check out all the information and benefits of the portal here.

Keep selection
Beta
New version
Current version